Problem

A flat coupon 12.5 mm wide and 3 mm thick with a 50 mm gage length is recorded in kN and mm. Slack in the load train adds extension while the force is still small, so the curve starts with a toe. Find the strain zero, the modulus and the 0.2 % offset yield strength.

Inputs to Enter

  • Data kind: force and extension, flat specimen; force in kN, extension in mm; 255 seeded illustrative rows with a header line (the fourth Try this case)
  • Width 12.5 mm, thickness 3 mm, gage length 50 mm, offset 0.2 %; toe compensation applied (the default); unit system SI for the values below
Open the Tensile Test Report tool

Answers

  • Original area 12.5 × 3.0 = 37.5 mm²
  • Elastic fit: rows 6 to 24 of the box, above the toe and below the knee, E = 70.27 GPa (generated with 72.0 GPa: 2.4 % low)
  • The fitted line meets zero stress at 0.2165 % strain, and every strain is counted from there (the record was generated with 0.110 mm of slack, 0.22 % of 50 mm)
  • 0.2 % offset yield strength 293.0 MPa (model value 291.6 MPa); ultimate strength 442.5 MPa
  • Strain at the end of the record 16.50 %, permanent part 15.92 %; without toe compensation every strain would read 0.22 % higher, and the yield strength would be the same
  • Strain hardening n = 0.129, K = 658.7 MPa (generated with n = 0.130, K = 660 MPa)

Notes

Open this case in the tool: /analysis-tools/structures/materials/tensile-test-report/?try=toe-region-slack (it opens in U.S. units; choose SI for the values above). Seeded synthetic data. The record has no rows after the break, so its last row is taken as the fracture point.