Tools › Structures › Materials › Tensile Test Report


Tensile Test Report

Paste the rows of a tension test (force and extension, or stress and strain) and get the report: modulus of elasticity from a fitted line, 0.2 % offset yield strength with the construction drawn, ultimate strength, uniform and total elongation, modulus of resilience, toughness, true stress and strain, and the strain-hardening exponent. The elastic part of the record is found by a stated rule that copes with noise, a toe region and a yield point. The page prints as a lab report: figures, the data table and every formula with its numbers.

  • Pasted rows, no file upload: force and extension with the specimen dimensions, or stress and strain, in the units of your record

  • The offset construction drawn and labeled: fitted elastic line, offset line, the intersection with the yield value, ultimate and fracture marked

  • Elongation, reduction of area, modulus of resilience and toughness, true stress and strain, strain-hardening exponent n and coefficient K

  • Upper and lower yield point found when the record has one; a toe region is removed by shifting the strain zero to the fitted line

Tensile Test Report


Unit System: /

/

Test record (one row per reading)








Specimen





Yield definition and report heading




Elastic fit and corrections







After fracture (measured on the broken specimen)





Comparison values (optional, typed from your specification or handbook)





×

Tensile Test Report

Tensile Test Report: From Pasted Rows to Modulus, Yield, Ultimate, Elongation and Toughness

The tool takes the rows of one tension test (force and extension with the specimen dimensions, or stress and strain) and reduces them to the numbers a test report carries: modulus of elasticity, offset yield strength, ultimate strength, elongation, modulus of resilience, toughness, and the true stress-strain curve with its strain-hardening exponent. It draws the stress-strain diagram with the offset construction on it and prints the formulas with your numbers.

The idea: one diagram, a handful of points on it

A stress-strain curve with the fitted elastic line, a parallel line offset by 0.2 percent strain that meets the curve at the yield strength, the maximum marked as the ultimate strength, the fracture point, the triangle of the modulus of resilience and the area under the curve as the toughness
Figure 1: The stress-strain diagram and what is read from it. A schematic: the elastic strain and the offset are drawn about ten times too wide.

A testing machine pulls a specimen and records the force and how much a marked length (the gage length) has stretched. Dividing the force by the original cross-section and the stretch by the original gage length gives a curve that belongs to the material and not to the size of the specimen. The first part of the curve is a straight line: the material is elastic, and the slope of the line is the modulus of elasticity. Then the curve bends over (yielding), climbs more slowly to a maximum (the ultimate strength), and the specimen necks and breaks.

Most metals bend over gradually, so there is no single point where yielding "starts". The agreed definition is the stress at which the specimen has taken a small permanent strain, 0.2 % by custom: draw a line parallel to the elastic line, 0.2 % strain to its right, and read the stress where it meets the curve (MIL-HDBK-5J, section 1.4.4.3).

The equations

QuantityFormulaNote
Engineering stressσ = F ÷ A0A0 = π d0² ÷ 4 (round) or w0 t0 (flat): the original area, whatever the specimen has become
Engineering strainε = x ÷ L0extension over the original gage length
Modulus of elasticityE = Σ(ε − ε̄)(σ − σ̄) ÷ Σ(ε − ε̄)²least-squares slope over the rows of the elastic part
Strain zero (toe compensation)ε0 = ε̄ − σ̄ ÷ Ewhere the fitted line meets zero stress; strains are counted from there
Offset lineσ = E (ε − ε0 − 0.002)0.002 = 0.2 %; the yield strength is the stress where the curve first meets it
Plastic strain of a rowεp = ε − ε0 − σ ÷ Eits distance to the right of the fitted line
Ultimate tensile strengthStu = Fmax ÷ A0the largest stress of the record
Elongation from the recordεf − σf ÷ Estrain at fracture less the elastic part, which springs back
Elongation after fracture(Lf − L0) ÷ L0from the gage marks of the broken specimen, halves fitted together
Reduction of area(A0 − Af) ÷ A0Af the smallest area at the fracture
Modulus of resilienceUr = Sty² ÷ (2 E)elastic energy per unit volume at the yield strength
ToughnessWt = Σ ½ (σi + σi−1)(εi − εi−1)area under the curve to fracture, trapezoid rule
True stress, true strainσt = σ (1 + ε), εt = ln(1 + ε)up to the maximum force only
Strain hardeningσt = K εtpn, with εtp = εt − σt ÷ En and ln K are the slope and intercept of ln σt against ln εtp, from yield to the maximum force
Ramberg-Osgood parameterεp = 0.002 (σ ÷ Sty)nn is the reciprocal of the slope of ln σ against ln εp for plastic strains from 0.02 % to 0.2 % (MIL-HDBK-5J, section 9.8.4.1.2)

How the elastic part is found

Real records are noisy, often start with a toe (slack and seating add extension before the specimen takes load), and end their straight part at a knee or a yield point. Picking the straight part by eye is where two people get two moduli from one test. The tool uses a rule adapted from the method described in NIST Technical Note 1679 (section 4.3):

  1. The knee. Take the strain of the first row at or above 5 % of the maximum stress. From the point at that strain and 20 % of the maximum stress, draw a line to every later row up to the maximum; the row that gives the steepest line is the knee (the line is tangent to the curve there).
  2. The steepest reliable run. Among all runs of consecutive rows between the 5 % row and the knee that hold at least a fifth of those rows (and at least five rows), fit a line to each and take the run whose slope, less four standard errors of that slope, is largest. A toe at the bottom and yielding at the top both lower the slope, so the elastic part is the steepest part of the curve; the standard error is subtracted so that a short run that is steep by chance does not win.
  3. Widening. The run is extended at both ends while rows stay within two residual standard deviations of its line (at least 0.1 % of the knee stress), stopping where two rows in a row fall outside; the line is fitted again, and this is repeated until the window stops changing.

The technical note takes the run with the lowest residual scatter and widens it once by one standard error; steps 2 and 3 are this page's changes, made because short runs won that contest by chance on noisy records. The technical note was written for compression tests of an aluminum alloy; the tool applies the same idea to tension records. You can set the strain range by hand in Advanced mode.

On seeded synthetic records with known answers the rule returns the modulus within about 1 % for clean records and about 3 % with moderate noise or a toe; the yield strength within about 1 %.

Other rules the tool states and uses

  • Fracture. If the record continues after the break, it is cut at the first row after the maximum whose stress is under 25 % of the maximum; the fracture point is the last row before the fall of more than 5 % of the maximum per row that leads there.
  • Yield point. A row that is the highest so far and is followed by three rows all lower by more than 0.5 % of its stress (and five times the scatter of the elastic fit), before the curve meets the offset line, is the upper yield strength. The lower yield strength is the lowest stress after it and before the curve rises above it again.
  • Strain at the maximum force. The top of a ductile curve is flat, and noise decides which row is highest; the strain is taken at the middle of the rows whose stress is within 0.5 % of the maximum.
  • Figures. At most 1,500 rows are drawn (every k-th row and the marked rows). Every result uses all rows; at most 5,000 are read.

What it assumes

  • The rows are in the order recorded and tension is positive.
  • The extension is that of the gage length entered. An extensometer measures it directly; crosshead travel also contains the stretch of the rest of the specimen, the grips and the machine.
  • The specimen deforms uniformly up to the maximum force (true stress and strain) and the material is elastic along the fitted line.
  • One specimen. The tool computes no averages and no statistics.

When it misleads

  • Crosshead data. A modulus from crosshead travel is the stiffness of the whole load train (specimen ends, grips, machine) and comes out too low, sometimes by a large factor. The yield strength by offset is still close, because the offset line is drawn from the fitted line, whatever its slope.
  • A curve that bends from the start (cast iron, annealed copper, some stainless steels) has no straight part; the fitted line is then a chord and the modulus depends on the rows it covers.
  • Few rows in the elastic part. With five or six rows the slope can be several percent off. Record more rows at the start of the test.
  • Elongation from the record is not the elongation after fracture of a test standard unless the extensometer stayed on to fracture and the neck formed inside its gage length. Total elongation also depends on the gage length, so values over different gage lengths cannot be compared.
  • Toughness here is the area under a tension curve. It is not fracture toughness and not an impact energy.
  • The strain-hardening law is a straight line forced through a log-log plot; many metals curve there, and n then depends on the strain range.

Common mistakes

  • Drawing the offset line from the origin of a record that has a toe. The line is offset from the fitted elastic line, not from the first data point.
  • Entering strain in percent where a ratio is expected (or the reverse): the modulus comes out a hundred times off.
  • Using the current (necked) diameter for the stress. Engineering stress always uses the original area.
  • Using the total length of the specimen, or the distance between the grips, as the gage length of an extensometer reading.
  • Reading the ultimate strength at fracture. It is the maximum of the curve, which for a ductile metal comes well before fracture.
  • Applying σ (1 + ε) beyond the maximum force. After necking begins the strain is no longer uniform and the formula does not hold.
  • Reporting a modulus to four figures. A tension test gives it to a few percent; a modulus test uses a more sensitive extensometer and a different procedure.
  • Confusing the Ramberg-Osgood parameter with the strain-hardening exponent: one is roughly the reciprocal of the other, and they are fitted over different strain ranges.

Test standards (ASTM E8/E8M for the test, E111 for the modulus, E646 for the strain-hardening exponent) set specimen shapes, speeds, extensometer classes and rounding; they are cited here and not reproduced. The definitions on this page follow MIL-HDBK-5J, a U.S. government handbook.




References

U.S. Department of Defense (2003). Metallic Materials and Elements for Aerospace Vehicle Structures. MIL-HDBK-5J, Department of Defense, Washington, DC.

Luecke, W. E., Ma, L., Graham, S. M., and Adler, M. A. (2009). Repeatability and Reproducibility of Compression Strength Measurements Conducted According to ASTM E9. NIST Technical Note 1679, National Institute of Standards and Technology, Gaithersburg, MD.

Luecke, W. E., Banovic, S. W., and McColskey, J. D. (2011). High-Temperature Tensile Constitutive Data and Models for Structural Steels in Fire. NIST Technical Note 1714, National Institute of Standards and Technology, Gaithersburg, MD.

Ramberg, W., and Osgood, W. R. (1943). Description of Stress-Strain Curves by Three Parameters. NACA Technical Note 902, National Advisory Committee for Aeronautics, Washington, DC.

Hollomon, J. H. (1945). "Tensile Deformation." Transactions of the American Institute of Mining and Metallurgical Engineers, Vol. 162, pp. 268–290.

ASTM International (2022). Standard Test Methods for Tension Testing of Metallic Materials. ASTM E8/E8M-22, ASTM International, West Conshohocken, PA.

ASTM International (2017). Standard Test Method for Young's Modulus, Tangent Modulus, and Chord Modulus. ASTM E111-17, ASTM International, West Conshohocken, PA.

ASTM International (2016). Standard Test Method for Tensile Strain-Hardening Exponents (n-Values) of Metallic Sheet Materials. ASTM E646-16, ASTM International, West Conshohocken, PA.


DISCLAIMER: The methods and calculation on aNOWysis.com are provided as means to educate the reader. There is no warranty, expessed or implied, as to the relevance or accuracy of the methods or calculations. All calculations should be checked by a qualified analyst for appropriateness and accuracy. We will not be held liable for any damages, injuries or deaths caused by using methods or calculations from this site.