Tools › Structures › Materials › Tensile Test Report › Example
MIL-HDBK-5J Table 9.8.4.1.1: the 0.2 % yield strength and the strain departures of a typical stress-strain curve
| Tool | Tensile Test Report |
| Source | U.S. Department of Defense (2003). Metallic Materials and Elements for Aerospace Vehicle Structures. MIL-HDBK-5J, Department of Defense, Washington, DC. Section 9.8.4.1.1, Table 9.8.4.1.1 (page 9-185). |
| Level | Professional |
Problem
The handbook builds a typical stress-strain curve from strain departures: at departures of 0, 20, 40, 100, 500, 1,000, 2,000 and 2,200 microstrain from the modulus line it lists the product-average stress and the total strain. Paste those eight rows under the straight part of the curve and recover the modulus, the departures and the 0.2 % yield strength.
Inputs to Enter
- Data kind: stress and strain; stress in ksi, strain in microstrain
- Rows of the straight part, on the line through the origin and the first printed row: 0, 0; 5.329, 502.8; 10.658, 1005.5; 15.986, 1508.2; 21.315, 2011.0; 26.644, 2513.8; 31.973, 3016.5; 37.301, 3519.2
- Printed rows (stress in ksi, total strain in microstrain): 42.63, 4022; 47.95, 4544; 50.12, 4768; 53.22, 5121; 59.27, 6092; 61.72, 6823; 64.00, 8038; 64.31, 8267
- Offset 0.2 %
Answers
- Modulus 42.63 ksi / 0.004022 = 10.60 Msi, fitted to the nine rows of the straight part (the handbook's elastic strains use the same value)
- Plastic strain of the printed rows (strain less stress / E): 0, 20, 40, 100, 500, 1,000, 2,000 and 2,200 microstrain, the printed departures to within 1.5 microstrain
- The 0.2 % offset line meets the curve at the row with 2,000 microstrain of departure: yield strength 64.00 ksi, the value the table marks as the product average yield strength
- Modulus of resilience 64,000² / (2 × 10,599,241) = 193.2 psi (in-lb/in³)
Notes
Enter the rows by hand (there is no preset for this case). The handbook's curve stops just past the yield strength, as its typical curves do, so the ultimate strength, fracture strain and toughness the page prints for these rows describe the last printed row and not a fracture. Checked in test_tensile_test_report.php.
More Examples for This Tool
- Tension test of a 0.505 in round bar: modulus, 0.2 % offset yield, ultimate strength, elongation and toughness from 236 force-extension rows
- Tension test with a yield point: upper and lower yield strength of a steel-like record
- A brittle record that breaks before the 0.2 % offset line: no offset yield strength
- Toe compensation: a flat coupon whose record starts with 0.11 mm of slack