Tools › Materials › Magnesium Alloy › ZE41A-T5 Sand casting

ZE41A-T5 Sand casting: MIL-HDBK-5J Design Allowables

Material classMagnesium Alloy
Alloy / temper / formZE41A / T5 / Sand casting
SpecificationsAMS 4439
HandbookMIL-HDBK-5J, 31 January 2003, section 4.3.6.0, Table 4.3.6.0(b) (pdf page 49 of the chapter file)
Dimension bands1
Density1816 kg/m³

Design Mechanical and Physical Properties (room temperature)

Converted from the handbook table (ksi, Msi, lb/in³) and rounded to 4 significant figures; dimension bands in inches with mm in parentheses. Bases: A and B are statistical minimums (99 % and 90 % probability at 95 % confidence), S the specification minimum. Grain directions: L longitudinal, LT long transverse, ST short transverse.

Dimension bandall
SpecificationAMS 4439
BasisS
Ftu, MPa179.3
Fty, MPa120.7
Fcy, MPa103.4
Fsu, MPa117.2
Fbru (e/D = 1.5), MPa262
Fbru (e/D = 2.0), MPa337.8
Fbry (e/D = 1.5), MPa213.7
Fbry (e/D = 2.0), MPa241.3
e, %2
E, GPa44.82
Ec, GPa44.82
G, GPa16.55
ν0.35
ρ, kg/m³1816

Effect of Temperature

Percent of the room-temperature value against temperature, digitized from the handbook figures (the shortest exposure of each figure, every 10 °F). Strength curves give the allowable at temperature; "after exposure" curves give the room-temperature property after a soak at that temperature.

Strength allowables at temperature, percent of room temperature

Moduli at temperature

°CF_tuF_ty
3897.790.1
9385.988.6
14972.680.9

Factors in percent of the room-temperature allowable.

Source and Use

U.S. Department of Defense (2003). Metallic Materials and Elements for Aerospace Vehicle Structures. MIL-HDBK-5J, 31 January 2003 (public domain). The values are the handbook's design allowables as extracted from the chapter tables; check the printed table before use in a certified analysis, and note that MIL-HDBK-5J was superseded by MMPDS, whose later editions may differ. No warranty is given.