Ti-10V-2Fe-3Al-Solution treated and aged (950-1000 F) Hand forging: MIL-HDBK-5J Design Allowables
show SI units (MPa, GPa, kg/m³) open the MIL-HDBK-5J tool compare against temperature find alternatives
| Material class | Titanium |
| Alloy / temper / form | Ti-10V-2Fe-3Al / Solution treated and aged (950-1000 F) / Hand forging |
| Specifications | AMS 4986 |
| Handbook | MIL-HDBK-5J, 31 January 2003, section 5.5.3.0, Table 5.5.3.0(c) (pdf page 142 of the chapter file) |
| Dimension bands | 2 |
| Density | 0.168 lb/in3 |
Design Mechanical and Physical Properties (room temperature)
As printed in the handbook table. Bases: A and B are statistical minimums (99 % and 90 % probability at 95 % confidence), S the specification minimum. Grain directions: L longitudinal, LT long transverse, ST short transverse.
| Dimension band | 0–3 in | 3.001–4.000 in | |
|---|---|---|---|
| Specification | AMS 4986 | AMS 4986 | |
| Basis | S | S | |
| Ftu, ksi | L | 160 | 160 |
| LT | 160 | 160 | |
| Fty, ksi | L | 145 | 145 |
| LT | 145 | 145 | |
| Fcy, ksi | L | 154 | … |
| LT | … | … | |
| Fsu, ksi | L | 97 | … |
| LT | 97 | … | |
| Fbru (e/D = 1.5), ksi | L | 241 | … |
| LT | 241 | … | |
| Fbru (e/D = 2.0), ksi | L | 293 | … |
| LT | 293 | … | |
| Fbry (e/D = 1.5), ksi | L | 218 | … |
| LT | 218 | … | |
| Fbry (e/D = 2.0), ksi | L | 245 | … |
| LT | 245 | … | |
| e, % | L | 6 | 6 |
| LT | 6 | 6 | |
| E, Msi | 15.9 | 15.9 | |
| Ec, Msi | 16.3 | 16.3 | |
| ρ, lb/in3 | 0.168 | 0.168 | |
Effect of Temperature
The handbook maps no temperature-effect figure to this table.
Other Ti-10V-2Fe-3Al Tables
Source and Use
U.S. Department of Defense (2003). Metallic Materials and Elements for Aerospace Vehicle Structures. MIL-HDBK-5J, 31 January 2003 (public domain). The values are the handbook's design allowables as extracted from the chapter tables; check the printed table before use in a certified analysis, and note that MIL-HDBK-5J was superseded by MMPDS, whose later editions may differ. No warranty is given.