MP35N-Solution treated and cold drawn Bar: MIL-HDBK-5J Design Allowables
show SI units (MPa, GPa, kg/m³) open the MIL-HDBK-5J tool compare against temperature find alternatives
| Material class | Miscellaneous |
| Alloy / temper / form | MP35N / Solution treated and cold drawn / Bar |
| Specifications | AMS 5844 |
| Handbook | MIL-HDBK-5J, 31 January 2003, section 7.4.1.0, Table 7.4.1.0(c) (pdf page 23 of the chapter file) |
| Dimension bands | 2 |
| Density | 0.304 lb/in3 |
Design Mechanical and Physical Properties (room temperature)
As printed in the handbook table. Bases: A and B are statistical minimums (99 % and 90 % probability at 95 % confidence), S the specification minimum. Grain directions: L longitudinal, LT long transverse, ST short transverse.
| Dimension band | dia 0–1 in | dia 1.001–1.750 in | |
|---|---|---|---|
| Specification | AMS 5844 | AMS 5844 | |
| Basis | S | S | |
| Ftu, ksi | L | 260 | 260 |
| Fty, ksi | L | 230 | 230 |
| Fsu, ksi | L | 145 | … |
| e, % | L | 8 | 8 |
| E, Msi | 34 | 34 | |
| G, Msi | 11.7 | 11.7 | |
| ρ, lb/in3 | 0.304 | 0.304 | |
Effect of Temperature
Percent of the room-temperature value against temperature, digitized from the handbook figures (the shortest exposure of each figure, every 10 °F). Strength curves give the allowable at temperature; "after exposure" curves give the room-temperature property after a soak at that temperature.
Moduli at temperature
Elongation and exposure effects
Other MP35N Tables
- MP35N-Solution treated, cold drawn, and aged Bar (Table 7.4.1.0(b))
Source and Use
U.S. Department of Defense (2003). Metallic Materials and Elements for Aerospace Vehicle Structures. MIL-HDBK-5J, 31 January 2003 (public domain). The values are the handbook's design allowables as extracted from the chapter tables; check the printed table before use in a certified analysis, and note that MIL-HDBK-5J was superseded by MMPDS, whose later editions may differ. No warranty is given.