7175-T7452 Hand forging: MIL-HDBK-5J Design Allowables
show SI units (MPa, GPa, kg/m³) open the MIL-HDBK-5J tool compare against temperature find alternatives
| Material class | Aluminum |
| Alloy / temper / form | 7175 / T7452 / Hand forging |
| Specifications | AMS 4149 and AMS-A-22771 |
| Handbook | MIL-HDBK-5J, 31 January 2003, section 3.7.8.0, Table 3.7.8.0(c) (pdf page 442 of the chapter file) |
| Dimension bands | 5 |
| Density | 0.101 lb/in3 |
Design Mechanical and Physical Properties (room temperature)
As printed in the handbook table. Bases: A and B are statistical minimums (99 % and 90 % probability at 95 % confidence), S the specification minimum. Grain directions: L longitudinal, LT long transverse, ST short transverse.
| Dimension band | 1.001–2.000 in | 2.001–3.000 in | 3.001–4.000 in | 4.001–5.000 in | 5.001–6.000 in | |
|---|---|---|---|---|---|---|
| Specification | AMS 4149 and AMS-A-22771 | AMS 4149 and AMS-A-22771 | AMS 4149 and AMS-A-22771 | AMS 4149 and AMS-A-22771 | AMS 4149 and AMS-A-22771 | |
| Basis | S | S | S | S | S | |
| Ftu, ksi | L | 71 | 71 | 68 | 65 | 63 |
| LT | 69 | 69 | 67 | 64 | 61 | |
| ST | … | 67 | 65 | 63 | 60 | |
| Fty, ksi | L | 61 | 61 | 57 | 54 | 51 |
| LT | 58 | 58 | 55 | 52 | 49 | |
| ST | … | 54 | 51 | 49 | 46 | |
| Fcy, ksi | L | 58 | 58 | 55 | 52 | 49 |
| LT | 61 | 61 | 57 | 54 | 50 | |
| ST | 60 | 60 | 57 | 54 | 51 | |
| Fbru (e/D = 1.5), ksi | L | 102 | 102 | 99 | 95 | 90 |
| LT | 102 | 102 | 99 | 95 | 90 | |
| ST | 102 | 102 | 99 | 95 | 90 | |
| Fbru (e/D = 2.0), ksi | L | 133 | 133 | 130 | 124 | 118 |
| LT | 133 | 133 | 130 | 124 | 118 | |
| ST | 133 | 133 | 130 | 124 | 118 | |
| Fbry (e/D = 1.5), ksi | L | 80 | 82 | 80 | 76 | 72 |
| LT | 80 | 82 | 80 | 76 | 72 | |
| ST | 80 | 82 | 80 | 76 | 72 | |
| Fbry (e/D = 2.0), ksi | L | 95 | 98 | 95 | 92 | 87 |
| LT | 95 | 98 | 95 | 92 | 87 | |
| ST | 95 | 98 | 95 | 92 | 87 | |
| e, % | L | 9 | 9 | 9 | 8 | 8 |
| LT | 5 | 5 | 5 | 5 | 5 | |
| ST | … | 4 | 4 | 4 | 4 | |
| E, Msi | 10.2 | 10.2 | 10.2 | 10.2 | 10.2 | |
| Ec, Msi | 10.5 | 10.5 | 10.5 | 10.5 | 10.5 | |
| G, Msi | 3.9 | 3.9 | 3.9 | 3.9 | 3.9 | |
| ν | 0.33 | 0.33 | 0.33 | 0.33 | 0.33 | |
| ρ, lb/in3 | 0.101 | 0.101 | 0.101 | 0.101 | 0.101 | |
Effect of Temperature
The handbook maps no temperature-effect figure to this table.
Other 7175 Tables
- 7175-T66 Die forging (Table 3.7.8.0(b))
- 7175-T73511 Extrusion (Table 3.7.8.0(d))
- 7175-T74 Hand forging (Table 3.7.8.0(c))
- 7175-T74a,b Die forging (Table 3.7.8.0(b))
Source and Use
U.S. Department of Defense (2003). Metallic Materials and Elements for Aerospace Vehicle Structures. MIL-HDBK-5J, 31 January 2003 (public domain). The values are the handbook's design allowables as extracted from the chapter tables; check the printed table before use in a certified analysis, and note that MIL-HDBK-5J was superseded by MMPDS, whose later editions may differ. No warranty is given.