7050-T7452 Hand Forging: MIL-HDBK-5J Design Allowables
show SI units (MPa, GPa, kg/m³) open the MIL-HDBK-5J tool compare against temperature find alternatives
| Material class | Aluminum |
| Alloy / temper / form | 7050 / T7452 / Hand Forging |
| Specifications | AMS 4108 and AMS-A-22771 |
| Handbook | MIL-HDBK-5J, 31 January 2003, section 3.7.4.0, Table 3.7.4.0(d) (pdf page 328 of the chapter file) |
| Dimension bands | 7 |
| Density | 0.102 lb/in3 |
Design Mechanical and Physical Properties (room temperature)
As printed in the handbook table. Bases: A and B are statistical minimums (99 % and 90 % probability at 95 % confidence), S the specification minimum. Grain directions: L longitudinal, LT long transverse, ST short transverse.
| Dimension band | 0–2 in | 2.001–3.000 in | 3.001–4.000 in | 4.001–5.000 in | 5.001–6.000 in | 6.001–7.000 in | 7.001–8.000 in | ||
|---|---|---|---|---|---|---|---|---|---|
| Specification | AMS 4108 and AMS-A-22771 | AMS 4108 and AMS-A-22771 | AMS 4108 and AMS-A-22771 | AMS 4108 and AMS-A-22771 | AMS 4108 and AMS-A-22771 | AMS 4108 and AMS-A-22771 | AMS 4108 and AMS-A-22771 | ||
| Basis | S | S | S | S | S | A | B | S | |
| Ftu, ksi | L | 72 | 72 | 71 | 70 | 69 | 68 | 71 | 67 |
| LT | 71 | 70 | 70 | 69 | 68 | 67 | 70 | 66 | |
| ST | … | 67 | 67 | 66 | 66 | 65 | 69 | 64 | |
| Fty, ksi | L | 63 | 62 | 61 | 60 | 59 | 56 | 61 | 57 |
| LT | 61 | 60 | 59 | 58 | 56 | 54 | 59 | 52 | |
| ST | … | 55 | 55 | 54 | 53 | 51 | 56 | 50 | |
| Fcy, ksi | L | 63 | 62 | 61 | 60 | 58 | 56 | 61 | 54 |
| LT | 64 | 63 | 62 | 61 | 59 | 57 | 62 | 55 | |
| ST | … | 63 | 61 | 60 | 58 | 56 | 61 | 54 | |
| Fsu, ksi | L | 42 | 41 | 41 | 41 | 40 | 40 | 41 | 39 |
| LT | 42 | 41 | 41 | 41 | 40 | 40 | 41 | 39 | |
| ST | … | 41 | 41 | 41 | 40 | 40 | 41 | 39 | |
| Fbru (e/D = 1.5), ksi | L | 98 | 97 | 97 | 96 | 94 | 93 | 97 | 91 |
| LT | 98 | 97 | 97 | 96 | 94 | 93 | 97 | 91 | |
| ST | … | 97 | 97 | 96 | 94 | 93 | 97 | 91 | |
| Fbru (e/D = 2.0), ksi | L | 131 | 129 | 129 | 127 | 125 | 123 | 129 | 121 |
| LT | 131 | 129 | 129 | 127 | 125 | 123 | 129 | 121 | |
| ST | … | 129 | 129 | 127 | 125 | 123 | 129 | 121 | |
| Fbry (e/D = 1.5), ksi | L | 86 | 84 | 83 | 82 | 79 | 76 | 83 | 73 |
| LT | 86 | 84 | 83 | 82 | 79 | 76 | 83 | 73 | |
| ST | … | 84 | 83 | 82 | 79 | 76 | 83 | 73 | |
| Fbry (e/D = 2.0), ksi | L | 101 | 100 | 98 | 96 | 93 | 90 | 98 | 86 |
| LT | 101 | 100 | 98 | 96 | 93 | 90 | 98 | 86 | |
| ST | … | 100 | 98 | 96 | 93 | 90 | 98 | 86 | |
| e, % | L | 9 | 9 | 9 | 9 | 9 | 9 | 9 | 9 |
| LT | 5 | 5 | 5 | 4 | 4 | 4 | 4 | 4 | |
| ST | … | 4 | 4 | 3 | 3 | 3 | 3 | 3 | |
| E, Msi | 10.2 | 10.2 | 10.2 | 10.2 | 10.2 | 10.2 | 10.2 | 10.2 | |
| Ec, Msi | 10.6 | 10.6 | 10.6 | 10.6 | 10.6 | 10.6 | 10.6 | 10.6 | |
| G, Msi | 3.9 | 3.9 | 3.9 | 3.9 | 3.9 | 3.9 | 3.9 | 3.9 | |
| ν | 0.33 | 0.33 | 0.33 | 0.33 | 0.33 | 0.33 | 0.33 | 0.33 | |
| ρ, lb/in3 | 0.102 | 0.102 | 0.102 | 0.102 | 0.102 | 0.102 | 0.102 | 0.102 | |
Effect of Temperature
The handbook maps no temperature-effect figure to this table.
Other 7050 Tables
- 7050-T73511 Extrusion (Table 3.7.4.0(e))
- 7050-T74 Die forging (Table 3.7.4.0(c))
- 7050-T7451 Plate (Table 3.7.4.0(b))
- 7050-T74511 Extrusion (Table 3.7.4.0(e))
- 7050-T7452 Die forgings (Table 3.7.4.0(c))
- 7050-T7651 Plate (Table 3.7.4.0(b))
- 7050-T76511 Extrusion (Table 3.7.4.0(e))
Source and Use
U.S. Department of Defense (2003). Metallic Materials and Elements for Aerospace Vehicle Structures. MIL-HDBK-5J, 31 January 2003 (public domain). The values are the handbook's design allowables as extracted from the chapter tables; check the printed table before use in a certified analysis, and note that MIL-HDBK-5J was superseded by MMPDS, whose later editions may differ. No warranty is given.